Understanding the Injection Molding Cycle: Filling, Packing, Cooling, and Gate Freeze
1. Introduction
Plastic injection molding is more than simply melting plastic pellets and injecting them into a mold. It is a carefully controlled process involving material preparation, melt flow, pressure control, cooling, and part ejection.
Understanding each stage of the injection molding cycle is essential for achieving consistent part quality, reducing defects, improving production efficiency, and optimizing tooling design.
In this article, we explore the major stages of the injection molding process, explain the difference between filling and packing, and take a closer look at Gate Freeze — an important factor influencing sink marks, dimensional stability, and cycle time.

2. The Five Main Stages of the Injection Molding Cycle
A typical injection molding cycle consists of five main stages:
Plasticizing
Filling
Packing / Holding
Cooling
Mold Opening and Ejection
These stages repeat continuously during production, with each cycle producing one shot of molded parts.
Stage 1: Plasticizing
Plastic raw materials are typically supplied in pellet form and fed into the injection molding machine through a hopper.
Inside the heated barrel, a rotating screw transports the material forward. Heat from the barrel heaters, combined with mechanical shear generated by screw rotation, gradually melts the plastic.
The molten material accumulates in front of the screw, preparing for the next injection cycle.
Different materials require different processing conditions. ABS, PC, PA66, PPS, and other engineering plastics have different melting or processing temperature ranges, thermal characteristics, and moisture requirements.
Proper plasticizing is essential for achieving a consistent melt temperature and material condition.
Stage 2: Filling
Once sufficient molten plastic has accumulated, the screw moves forward and injects the material into the mold.
The melt typically flows through the following path:
Injection Unit → Nozzle → Sprue → Runner → Gate → Cavity
Each component plays a specific role in delivering molten plastic into the product cavity.
The objective of the filling stage is to fill the cavity within an appropriate time while maintaining a stable and controlled flow.
Poor filling conditions or mold design may result in defects such as:
Short Shot — incomplete filling
Flow Marks — visible flow patterns
Weld Lines — meeting lines between separate melt fronts
Air Traps — trapped air inside the cavity
Burn Marks — discoloration or damage caused by trapped air or excessive local heating
Gate location, runner design, injection speed, and mold venting all influence the filling process.

Stage 3: Packing / Holding
After the cavity has been substantially filled, the process transitions from filling to packing or holding.
Plastic materials shrink as they cool. During this stage, additional molten plastic is pushed into the cavity to compensate for volumetric shrinkage.
This helps reduce sink marks, internal voids, and dimensional variations.
It is important to distinguish between the two pressure stages:
Injection / Filling Pressure is primarily used to move molten plastic into the cavity.
Holding / Packing Pressure is applied after filling to compensate for material shrinkage while the plastic is cooling.
Packing pressure and packing time must be carefully controlled. Excessive pressure may cause flash, residual stress, dimensional variation, or excessive part weight.
Insufficient packing may result in sink marks, voids, or inconsistent dimensions.
However, packing can only remain effective while molten plastic can still flow through the gate.
This leads to an important concept: Gate Freeze.
3. What Is Gate Freeze?
Gate Freeze occurs when the plastic at the gate cools and solidifies to the point where effective material flow into the cavity is no longer possible.
The gate is often a relatively small and thin section of the mold, making it particularly sensitive to cooling.
As molten plastic enters the mold, heat is transferred from the plastic to the surrounding steel. The material near the gate gradually cools and solidifies, eventually restricting or stopping further material flow.
Once the gate is effectively sealed, additional holding pressure or holding time can no longer provide meaningful additional material to the cavity.
This is why understanding Gate Freeze is important when optimizing packing conditions.

Why Does Gate Freeze Time Vary?
Gate Freeze time is not determined by the material alone. It depends on several interacting factors.
1. Material Properties
Different plastics have different thermal properties, including thermal conductivity, specific heat capacity, and thermal diffusivity.
Crystalline materials such as PA66, POM, and PPS also exhibit crystallization behavior during cooling, which affects their solidification characteristics.
Amorphous materials such as ABS and PC behave differently during cooling.
Therefore, different materials may require different packing and cooling conditions.
2. Gate Design
Gate thickness, width, length, and geometry influence how quickly the plastic at the gate cools.
In general, a thinner gate tends to freeze earlier, while a thicker gate may maintain effective flow for longer under otherwise similar conditions.
However, a larger gate is not always better. Gate dimensions must also consider appearance, gate removal, filling behavior, and overall mold design.
3. Mold Temperature
The mold temperature affects heat transfer from the molten plastic.
Under otherwise similar conditions, a lower mold temperature generally accelerates cooling at the gate, potentially resulting in earlier gate freeze.
However, excessively low mold temperatures may negatively affect filling, weld line quality, surface appearance, and residual stress.

4. Melt Temperature
A higher melt temperature generally means more heat must be removed before the plastic at the gate becomes unable to flow.
Increasing melt temperature may extend the effective packing window, but it may also increase cooling requirements, cycle time, and the risk of material degradation if processing limits are exceeded.
5. Product and Mold Structure
Product wall thickness, flow length, gate location, and cooling channel arrangement influence the temperature distribution throughout the cavity.
A thick boss may remain hot and continue shrinking even when a thin gate has already frozen.
This is one of the reasons why thick sections located far from the gate may be particularly vulnerable to sink marks.
4. How Can Engineers Determine Gate Freeze Time?
Rather than estimating Gate Freeze time based only on experience, engineers can perform a practical experiment known as a Gate Seal Study or Gate Freeze Study.
The principle is simple:
If increasing holding time results in an increase in part weight, additional plastic is still entering the cavity.
Once part weight becomes nearly stable, the gate has likely reached its effective sealing point.
Example of a Gate Seal Study
Assume the holding pressure remains constant while holding time is gradually increased.
Holding Time | Part Weight |
1 second | 48.20 g |
2 seconds | 48.55 g |
3 seconds | 48.78 g |
4 seconds | 48.91 g |
5 seconds | 48.94 g |
6 seconds | 48.94 g |
7 seconds | 48.95 g |
In this example, part weight increases significantly during the early packing stages.
At approximately 5–6 seconds, the weight becomes nearly stable.
This suggests that the gate has reached its effective sealing point around this period.
Continuing to increase holding time beyond this point provides little additional material compensation and may unnecessarily increase the production cycle.
Why Is This Test Useful?
A Gate Seal Study helps engineers identify an appropriate holding time based on actual production behavior.
It can be used to optimize:
Holding Time
Part Weight
Sink Mark Performance
Dimensional Stability
Cycle Time
The test should be conducted under stable conditions, with consistent injection settings, holding pressure, material condition, and mold temperature.
Part weight stabilization is a practical indicator of gate sealing, but it does not automatically guarantee that all product quality requirements have been satisfied.
5. How Can Gate Freeze Time Be Extended?
When insufficient packing causes sink marks or other shrinkage-related problems, engineers may investigate ways to extend the effective packing window.
A. Mold Design Optimization
Increase Gate Thickness
Increasing gate thickness may slow cooling at the gate and extend the time during which molten plastic can enter the cavity.
However, the design must also consider gate appearance, gate removal, filling behavior, and potential cycle time changes.
Optimize Gate Location
Gate location influences flow direction, pressure loss, and the ability to pack critical areas.
For products containing thick bosses or ribs, a suitable gate location may help deliver molten plastic more effectively to these regions before the gate freezes.
Gate location should also consider weld line positions, appearance requirements, and filling balance.

B. Process Optimization
Adjust Melt Temperature
Within the material's recommended processing range, increasing melt temperature may extend the time before the gate becomes unable to transmit material.
However, a higher melt temperature may also increase cooling requirements and cycle time.
Adjust Mold Temperature
A higher mold temperature may slow cooling at the gate and extend the packing window.
However, the overall cooling cycle may also become longer.
Optimize Holding Pressure
Holding pressure influences the amount of material packed into the cavity while the gate remains open.
Increasing holding pressure may improve shrinkage compensation, but it does not necessarily extend Gate Freeze time.
Excessive pressure may cause flash, residual stress, dimensional variation, or excessive part weight.
The objective is to identify the appropriate pressure and time combination through controlled trials rather than simply increasing pressure or time.
6. Understanding Sink Marks Around a Plastic Boss
Sink marks are commonly observed around thick sections, bosses, ribs, and other areas where material accumulates.
Consider a plastic housing with a relatively thick boss.
During cooling, the thick section retains heat longer than the surrounding thinner wall. As the material cools and shrinks, the outer surface may be pulled inward, creating a visible sink mark.
The problem may involve several factors simultaneously:
Excessive local material accumulation
Thick boss wall design
Insufficient packing pressure
Insufficient packing time
Premature gate freeze
Inefficient cooling around the boss
Uneven cooling between different sections of the product
A proper investigation should therefore consider both product design and molding conditions.
Step 1: Review Boss Design
Engineers should evaluate whether the boss contains unnecessary material.
Possible design improvements include:
Reducing boss wall thickness
Coring out unnecessary material
Improving the transition between the boss and the main wall
Using ribs or gussets to provide structural support
Maintaining a more uniform wall thickness where practical
The objective is to reduce excessive material accumulation while maintaining the required structural strength.
Step 2: Review Packing Conditions
If the design is acceptable, engineers should investigate whether the packing process is sufficient.
Questions include:
Is the holding pressure adequate?
Is the holding time sufficient?
Is the gate freezing too early?
Is the gate size appropriate?
Is the gate location favorable for packing the boss?
Is cooling around the boss effective?
Extending holding time may help if the gate remains open and the existing packing time is insufficient.
However, if the gate has already frozen, increasing holding time will not effectively compensate for further shrinkage in the cavity.
Step 3: Review Cooling Conditions
The cooling system should be evaluated to determine whether heat is being removed effectively from the thick section.
Cooling channel location, distance from the boss, cooling circuit design, and local mold temperature may all influence the final result.
A balanced cooling system can help improve dimensional stability and reduce warpage.
7. The Relationship Between Product Design, Mold Design, and Process
Injection molding defects rarely result from a single factor.
A sink mark may originate from product design, but it may also be influenced by gate design, material selection, packing conditions, and cooling performance.
This is why effective troubleshooting requires a systematic approach.
A practical engineering workflow is:
l Identify the defect location and pattern.
l Review the product geometry and local wall thickness.
l Check for excessive material accumulation.
l Review gate location and gate dimensions.
l Evaluate holding pressure and holding time.
l Conduct a Gate Seal Study if necessary.
l Review the cooling system.
l Implement improvements and validate the results.
The best solution is not always to adjust the molding parameters.
Sometimes the most effective improvement is a product design change. In other cases, mold design or process optimization may provide the solution.
The key is to understand the root cause before making adjustments.
8. Conclusion
Understanding the injection molding cycle helps engineers and manufacturers identify the relationship between filling, packing, cooling, and part quality.
Gate Freeze is particularly important because it determines how long the mold cavity can receive additional material during packing.
By understanding the influence of material properties, gate dimensions, mold temperature, melt temperature, and product geometry, engineers can optimize packing conditions and avoid unnecessary holding time.
A Gate Seal Study provides a practical way to identify when additional packing no longer significantly increases part weight, helping improve process efficiency without compromising quality.
When sink marks appear around a boss, the investigation should begin with the product design and local material accumulation, followed by an evaluation of packing, gate freeze, and cooling conditions.
Good injection molding is not simply about adjusting machine parameters. It is about understanding the interaction between product design, mold design, material behavior, and process conditions.
At Opro-Tech, we believe that combining design knowledge with manufacturing experience is essential to delivering reliable tooling and high-quality plastic components.
Engineering Note: Actual processing parameters and design recommendations should always be validated based on the specific material, mold structure, product requirements, and production trials.